■ Overview
Low alloy structural steel S355G8+M,S355G8+M steel plate,S355G8+M steel sheet is Under European steel standard En 10225,S355G8 has two different types,aush as S355G8+M and S355G8+N,the main difference is the heat treatment when rolling.Oil and offshore platform steel plate S355G8+M shall be done TMCP when rolling,and S355G8+N shall be done Normalized heat treatment.These two oil and offshore steel grade shall be done low temperature under mins 40 centigrade and the minimum energy value shall be above 50J.
■ Full Data
Technical Requirements & Additional Services for S355G8+M steel plate:
♦ Z TEST (Z15,Z25,Z35)
♦ Low temperature impacting test
♦ Ultrasonic test under EN 10160,ASTM A435,A577,A578
♦ Issued Orginal Mill test certificate under EN 10204 FORMAT 3.1/3.2
♦ Shot blasting and Painting,Cutting and welding as per end user’s demands
♦ Z TEST (Z15,Z25,Z35)
♦ Low temperature impacting test
♦ Ultrasonic test under EN 10160,ASTM A435,A577,A578
♦ Issued Orginal Mill test certificate under EN 10204 FORMAT 3.1/3.2
♦ Shot blasting and Painting,Cutting and welding as per end user’s demands
■ Techicals
►Mechnical property for S355G8+M steel plate:
Thickness (mm) | |||||||
S355G8+M | ≤ 16 | > 16 ≤ 25 | > 25 ≤ 40 | > 40 ≤ 63 | > 63 ≤ 100 | > 100 | |
Yield strength (≥Mpa) | 355 | 355 | 345 | 335 | 325 | 325 | |
≤ 100 | > 100 | ||||||
Tensile strength (Mpa) | 470-630 | 470-630 |
►Chemical composition for S355G8+M steel plate (Ladle Analysis Max%)
Main chemical elements composition of S355G8+M steel plate | ||||||||
C | Si | Mn | P | S | Cr | Mo | Nb+V | Nb+V+Ti |
0.14 | 0.15-0.55 | 1.00-1.65 | 0.020 | 0.007 | 0.25 | 0.08 | 0.06 | 0.08 |
Ni | Alt | Cu | N | Nb | Ti | V | Cr+Mo+Ni+Cu | |
0.50 | 0.015-0.055 | 0.30 | 0.010 | 0.040 | 0.025 | 0.060 | 0.90 |