■ Overview
The highest tensile strength in normal shipbuilding steel,CCS Grade EH40,CCS EH40,CCS EH40 steel plate is normally used to build ships which are sailing in the bad surroudings.CCS Grade EH40 Marine steel plate,CCS Grade EH40 shipbuilding steel plate,CCS EH40 steel plate,CCS Grade EH40 ship plate,CCS Grade EH40 shipbuilding steel plate which are rolled under Normalised or Thermal Mechanical Control Processing.
■ Full Data
Technical Requirements & Additional Services for CCS EH40 steel plate:
♦ High tension test
♦ Z-Test (Z15,Z25,Z35)
♦ Low temperature impacting test
♦ Ultrasonic test under ASTM A435,A577,A578
♦ Cetificated by ABS,LR,GL,BV,DNV,KR,NK,CCS,RINA
♦ Issued Orginal Mill test certificate under EN 10204 FORMAT 3.1/3.2
♦ Shot blasting and Painting,Cutting and welding as per end user’s demands
♦ High tension test
♦ Z-Test (Z15,Z25,Z35)
♦ Low temperature impacting test
♦ Ultrasonic test under ASTM A435,A577,A578
♦ Cetificated by ABS,LR,GL,BV,DNV,KR,NK,CCS,RINA
♦ Issued Orginal Mill test certificate under EN 10204 FORMAT 3.1/3.2
♦ Shot blasting and Painting,Cutting and welding as per end user’s demands
■ Techicals
►Mechnical property for CCS Grade EH40 shipbuilding structual steel:
Yield strength (≥Mpa) | Tensile strength (Mpa) | Elongation in ≥,% | |
390 | 510-650 | 200mm | 50mm |
19 | 22 |
►Chemical composition for CCS Grade EH40 ship steel (Heat Analysis Max%)
Main chemical elements composition of CCS Grade EH40 | ||||||
C | Si | Mn | P | S | Al (acid) min. | Nb |
0.18 | 0.10-0.50 | 0.90-1.60 | 0.035 | 0.035 | 0.015 | 0.02-0.05 |
V | Ti | Cu | Cr | Ni | Mo | |
0.05-0.10 | 0.02 | 0.35 | 0.20 | 0.40 | 0.08 |